We measured the reflectivity of an Athena silicon pore optics sample coated with 10-nm thick iridium near the iridium L-edges (L3 , L2, and L1) in a step of 1.5 eV. The derived atomic scattering factor f2 was similar to a shape of the absorption coefficient μ near L3 and L2 obtained by previous x-ray absorption spectroscopy (XAS) measurements. The fine structures of f2 of L3 and L2 can be represented by a strong sharp line referred to as a white line (WL) and two weak lines at center energies of ∼17 and ∼31 eV from each edge energy. The branching ratio (L3 / L2) of the WL is >2, which reflects the initial core-electron states available for the L2 (2p1/2) and L3 (2p3/2) processes, and the ratio remains high to the energy of +7 . 5 eV from WL. The fine structure seen in L1 also has two weak lines, which were seen in XAS at L1-edge. Our measurements near L3, L2, and L1 edges demonstrated a different technique to provide atomic structural information as XAS. The ground calibration to measure fine structures near the edges may potentially be simplified using f2 estimated based on μ. |
1.IntroductionThe x-ray absorption fine structure (XAFS) is often measured with x-ray absorption spectroscopy (XAS) to find useful information on the environment (geometry) and electronic structure of the absorbing atoms. XAS is performed in a transmission setup, providing a direct measure of the linear x-ray attenuation coefficient . The x-ray absorption edge spectra of iridium, which is one of the elements having high electron density, such as Au, Pt, etc., have been obtained to reveal the fundamental characteristics of the material1–3. Clancy et al.1 (hereafter Clancy12) investigated spin-orbit coupling effects in a series of Ir- and Re-based compounds using XAS techniques and observed anomalously large branching ratios in all Ir-based compounds, indicating a very large expectation value for the spin-orbit operator in these systems. On the other hand, small oscillations are seen in the reflectance setup, referred to as the diffraction anomalous fine structure (DAFS). Stragier et al.4 studied the DAFS as a new x-ray structural technique and demonstrated that the DAFS measurements provide the same local atomic structural information as XAFS. They used XAFS standards to analyze the DAFS data by shifting the phase. Pickering et al.5 applied the Kramers–Kronig relation to the atomic scattering factors and and determined the scattering factor to fit the DAFS data. The scattering factor is suitable for research of XAFS because is related to the absorption coefficient : ,6 where , is the Planck’s constant, is the classical electron radius, and is the speed of light. However, the value in the wide energy band is required for calculating the value using the Kramers–Kronig relation. The atomic scattering factors and of iridium can be derived from the reflectance obtained by angular scan and/or energy scan without using the Kramers–Kronig relation. This is demonstrated by measurements on the ground for building the response function of the x-ray mirror (e.g., ASTRO-H7 and Chandra8). We measured the reflectance of a sample fabricated by employing ESAs silicon pore optics (SPO) technology in the high energy region from 9000 to 15,000 eV at the synchrotron radiation facility SPring-89 and obtained the atomic scattering factors of iridium near -edges with an energy pitch of 1.5 eV. We compare the fine structure with XAFS and show that the method using reflection is as effective as XAFS methods. In addition, it is becoming increasingly important to measure the fine structure of the atomic scattering factors because of the improvement in energy resolution of focal plane detectors in recent years.10,11 Although fine energy scans for measuring and near the edges are possible, estimating from can reduce the time required for ground calibration tests.7,9 In Sec. 2, we introduce our x-ray measurements and calculate the atomic scattering factors from the reflectance. In Sec. 3, we characterize the fine structure seen in the atomic scattering factor to compare the previous work on XAFS and then analyze the derived in a way similar to XAS. 2.X-Ray Measurement and Estimation of the Atomic Scattering Factors2.1.X-Ray MeasurementOur SPO sample was prepared at the coating facility dedicated for the Athena mirror production.12,13 The sample has a length and width of 110 and 49 mm, respectively. A 10-nm thick iridium thin film coating was deposited using DC magnetron sputtering. The details of the sample preparation are described in Awaki et al. 2021.9 We measured the x-ray reflectivity of the SPO sample at BL20B214 in SPring-8. The crystal plane of 311 of the Si double crystal monochromator15 was selected to monochromatize continuum x-rays in our experiment. The energy resolution () of the available x-ray beam is in the energy range from 9000 to 15,000 eV, and the energy scale was calibrated by measurements of the Cu -edge structure. We measured the intensity of a reflected x-ray on the SPO sample as well as the intensity of an incident x-ray and derived the reflectance , defined as the ratio of the intensity of a reflected x-ray to that of the incident x-rays. Since the reflectance is described as a function of the energy of the incident x-ray and grazing angle , we measured the reflectivity by performing angle and energy scans at fixed energies and fixed incident angles, respectively. In the energy scans, three fine pitch scans with an incident angle of 0.2, 0.32, and 0.4 deg were performed around the energies of the iridium L-edges in steps of 1.5 eV to clarify the iridium -shell structure of and . The scanning energy ranges are 11 to 11.5 keV for edge, 12.5 to 13 keV for edge, and 13.2 to 13.7 keV for edge. Figure 1 shows the reflectance obtained in the energy scans. We can clearly see small oscillations in the post-edge region. These small oscillations are referred to as DAFS. Angle scans were performed at x-ray energies of 11, 12, and 14 keV, spanning the range of the iridium -edges, specifically. The incident angle was scanned up to 1.5 deg in steps of 0.05 deg to measure the thickness of the iridium layer. 2.2.Estimation of the Atomic Scattering FactorsThe reflectance of a single thin layer can be calculated using the refractive indices of the thin layer and the substrate. By fitting the measured data with a single thin layer model, we can estimate the parameters describing the iridium layer, specifically, the thickness of the iridium layer (), interfacial roughness between the iridium layer and SPO substrate (), and the surface roughness of the iridium layer (). However, the angle data points in the energy scan were not enough to estimate the parameters. Thus, the fit to the angle scan data was used to identify the parameters describing the iridium layer, specifically, , , and . In this calculation, the loss of reflectance owing to roughness was considered as the Nevot–Croce factor,16 and the atomic weight and the corresponding mass density of iridium were taken as 192.22 and ,17 respectively. We employed an overlayer model, assumed as a hydrocarbon chain of the form with a density of (Graessle et al.8). The best-fit values were obtained from the angle scan. The details of the measurements are given in Awaki et al.9 In the fitting procedure of the energy scan data, , , and were set as constant at the weighted mean values of the best-fit values of the angle scan data (, , ). The thicknesses of the overlayer were set to be 0.9 nm because we found that an overlayer thickness of 0.9 nm led to a better fit to the data reported by Henke et al.6 Figure 2 shows the derived near the iridium -edges to clarify their structures. 3.Fine Structures Derived from the Atomic Scattering Factor f23.1.Comparison with the XANES Obtained from XASIt is known that the absorption coefficient of iridium near and edges contains three main features: (i) a sharp line feature known as “white line”18,19 (hereafter WL), (ii) a step-like edge feature, and (iii) a small wave-like feature.1,20 The scattering factor near and edges also shows these features (see Fig. 2). To confirm the similarity between by Clancy12 and our result , the Clancy12 data (arb. unit) was scaled to fit our data and then overlaid on our data in Fig. 2. Both data were found to be similar, including the small wave feature in the energy . The similarity suggests that (1) the fine structures of obtained from reflectance are consistent with XAFS obtained from XAS and (2) there is no apparent difference of optical characteristics between a thin iridium film formed by a DC magnetron sputter and an iridium powder with a purity of 99.99%. The similarity to Clancy12 can also be seen in the best-fit parameters of . Comparing the best-fit parameters obtained by Awaki et al.9 with previous works,1,20 the best-fit parameters (center energy and line width) of WL were consistent with previous works1,20 (see Table 1). Clancy12 also measured WL and estimated the branching ratio to be 3.2, which is larger than that of our result. In the fitting procedure by Clancy12, the line width of WL was fixed to the same line width as WL. Thus, we fitted the WL with the same line width as WL. The branching ratio is changed to , which is consistent with their result. Table 1L3 and L2 white lines.
3.2.Fine Structures of the Scattering Factor f2 Near L-EdgesThere are two distinct peaks ( and in Fig. 2) in the fine structures at and -edges, and these peaks are also seen in the x-ray absorption near edge structure (XANES) results obtained by previous works.1 Each peak was fitted with a Lorentzian model. The best-fit parameters are shown in Table 2. The center energy of each peak is represented by the energy from the absorption edge. Since the center energies and line widths of in the edge are consistent with those of in edge in the error region, p1 detected in edge is considered to be a transition to the same state as detected at edge. It would be the same for as for . Sham21 studied the x-ray absorption fine structures at -edges for 4d elements, Rh, Pd, and Ag, and there were prominent weak peaks at and in their absorption spectrum at the -edge for these materials. The two weak lines and in Fig. 2 would be assigned to peaks 2 to 4 () and 5 () in Table 1 of Sham.21 To find branching ratios of these lines, we fixed both the center energies and the line width () of the two peaks at the weighted mean values ( and 31.8 eV, and 4.6 eV for and , respectively) and fitted and with a Lorentzian model. The branching ratio of was larger than 2 but the error was large, while the branching ratio of was consistent with 2. Table 2Best fit parameters of two peaks in L-edge structure.
Error ranges represent 1σ confidence boundaries for a parameter of interest (χmin2+1). On the fine structure at the edge, there are two prominent peaks at and . The prominent lines are clearly seen in the of iridium the edge in the Materials Data Repository. Although Sham21 studied the -edge x-ray absorption properties of 4d noble metals, there were two clear peaks of absorption coefficient at about 18 and 40 eV from the edge in Fig. 8 of Sham,21 and these two peaks were associated with , and , respectively. This assignment of the two peaks will be helpful to consider the and assignments found in the iridium edge, although we cannot eliminate the possibility that might be similar to extended XAFS (EXAFS) due to the large line width of . 3.3.Ratio of the Scattering Factor f2 Between L2 and L3-EdgesThe measured step size, which presents the depth of an edge, of the edge was twice that of the edge. Since the step-like edge features are associated with the continuum transition, the ratio of the step size reflects the ratio, which is 1:2, of the initial core-electron states available for the () and () processes. On the other hand, the WL, which is associated with transition, has a branching ratio . We investigated how the ratio of the scattering factor () changes with energy offset from WL. At first, we estimated a floor value of in the energy region of from to , and then subtracted the floor value from the measured . Next, the measured was smoothed by applying savgol_filter in python 3.8.2 with a window length of 5 and an order of 2 to reduce scattering of the ratio due to poor statistics. Figure 3 shows the after subtraction of the floor value and the ratio of , where and are the at edge and edge, respectively. The solid line indicates the smoothed curve with savgol_filter. The energy is the energy from the center energy of WL, because the uncertainty of the edge energy in our fitting results makes a discrepancy of the energy between and regions, and then the discrepancy makes pseudo peaks in the ratio near WL. A typical error of the ratio at the energy is 0.14. The branching ratio around the energy of WL is about 2.4, which is significantly . The branching ratio remains large up to . This result is consistent with a larger line width of WL in than that in . In the energy region to 18 eV, the ratio is 2.1–2.2, which is slightly larger than 2. This result is also in agreement with the estimation of the results of the branching ratio of . Above 20 eV, the branching ratio becomes to be a mean value of 2.04 with a standard deviation of 0.05, which is consistent with the ratio of the density of states between and . 3.4.Fine Structures at ΔE >50 eV Seen in the Scattering Factor f2It is found that the structure of the data at is similar to that of the data (see Fig. 2). The similarity can also be seen in the constant ratio of at (see Fig. 4). The origin of the fine structure in EXAFS is the interference between the incoming and scattered photoelectron waves. The kinetic energy of a photoelectron wave is given by , where is the photon energy and is the edge energy. Interference patterns should depend on because the wavelength of a photoelectron is related to . Thus, the fine structure in EXAFS of is expected to be similar to that of . We supposed that the fine structure of the data is also similar to that of the data, but we did not see a clear similarity. If we shift the energy of the data by , we may see a weak similarity between the fine structures of and . 4.Discussion4.1.Measurement of the Atomic Scattering FactorsWe have demonstrated that the fine structure obtained from the reflectance is similar to the XANES results obtained using XAS. This confirms the relationship between and and shows that can be estimated from . Estimating from may lead to reducing the time for the ground calibration of an x-ray mirror because the detailed structure of near the absorption edge is measured without a fine energy scan of the reflectance. In addition, because is accurately determined via XAS, the error margin in value obtained using is small. We demonstrate this possibility by fixing in our data. Figure 4 shows the error of when was fixed. It is found that the error in the value decreased by 0.3 to 0.8 times. As the critical angle for iridium at 12 keV is , the x-ray reflectivity at an incident angle of 0.4 deg at an energy of 12 keV or less is not sufficiently low (Fig. 1). Thus, the uncertainty in the value is large when is set to a free parameter. Using may be worthwhile when using data wherein the incident angles are close to or below the critical angle. 4.2.XAFS MeasurementOur result suggests that the 10-nm-thick iridium formed by the DC magnetron sputtering device has almost the same optical property as that of iridium powder. This result indicates that a study of XAFS is possible with a thin layer instead of powder. The reflectance measurements will be useful for fine structure research on thin atomic layer samples that are difficult to do with XAS technique. For thin films, the absorption coefficient is estimated by measuring the intensity of a fluorescence line (fluorescence XAFS measurements22,23). However, the self-absorption effect causes distortion in the measured spectra in fluorescence line, and a correction for this distortion is needed.22 In addition, a sufficient intensity of fluorescence line is required to obtain with a high signal-to-noise ratio. Our reflectance measurement is an alternative method to estimate the absorption coefficient. The similarity between and suggests that the effects observed in the fluorescence XAFS measurements are small. We have provided the fine structures of in the energy region from iridium L-edges (, and ). The properties of the two peaks are similar to those of material obtained by Sham 1985. We have also calculated the ratio in the energy range . The ratio is about 2.4 in the energy range , and as the photon energy increases, the ratio decreases; at the energy , the ratio comes to the mean value of , which is consistent with the ratio of the density of states between and . The origin of the fine structure in EXAFS is the interference between the incoming and scattered photoelectron waves. Thus, each fine structure in the EXAFS region can be compared because we obtained the fine structures of the -edges (, and ). The fine structure of is, as expected, similar to that of , but the fine structure of is not similar to that of . If we shift the energy of the data by , we may see a weak similarity between the fine structures of and . This shift may be because of the difference between the transition () and the transition (). Detailed analysis using high quality data is required to investigate the fine structures of iridium -edges. 5.ConclusionWe measured the reflectance of an SPO plate coated with an iridium layer having a thickness of 10 nm at Spring-8 in the energy range covering all iridium -edges. We have shown that the shape of the fine structures of near and edges are remarkably similar to those in previous works on XAFS. The similarity suggests that we could obtain for a reflector substrate with an Ir film with a thickness of 10 nm by measuring the reflectance. In measuring the fine structure of the metal on the reflective surface at the fine energy pitch, the method used in this study leads to a reduction in the time of the ground calibration. Moreover, as the value of is well determined via XAS, the error in is reduced using estimated based on . By comparing of , and , the ratio of values corresponding to and was found close to 2 and exceeded 2 near WL. Regarding the structure of XAFS, and are similar, and the energy apparently shifts between and . This is probably because the final state of the transition is for and , whereas it is for . Further detailed analyses of the fine structures using an analysis tool such as Demeter 0.9.26 are therefore required.24 AcknowledgmentsThe X-ray measurement was performed at BL20B2 in SPring-8 with the approval of the Japan Synchrotron Radiation Research Institute (JASRI) (Proposal No. 2018B1106 (YM)). We used the MINUIT software package developed by CERN for the fitting procedure. This work was financially supported by JSPS KAKENHI [Grant Nos. 20H00175 (HM) and 21K18152(HA)]. We would like to thank Editage for English language editing. The authors have no relevant financial interests in the manuscript and no other potential conflicts of interest to disclose. ReferencesJ. P. Clancy et al.,
“Spin-orbit coupling in iridium-based 5d compounds probed by x-ray absorption spectroscopy,”
Phys. Rev. B, 86 195131 https://doi.org/10.1103/PhysRevB.86.195131
(2012).
Google Scholar
T. Anniyev et al.,
“Complementarity between high-energy photoelectron and L-edge spectroscopy for probing the electronic structure of 5d transition metal catalysts,”
Phys. Chem. Chem. Phys., 12 5694
–5700 https://doi.org/10.1039/b926414k PPCPFQ 1463-9076
(2010).
Google Scholar
A. Wach, J. Sá and J. Szlachetkoa,
“Comparative study of the around-Fermi electronic structure of 5d metals and metal-oxides by means of high-resolution X-ray emission and absorption spectroscopies,”
J. Synchrotron. Radiat., 27 689
–694 https://doi.org/10.1107/S1600577520003690 JSYRES 0909-0495
(2020).
Google Scholar
H. Stragier et al.,
“Diffraction anomalous fine structure: a new x-ray structural technique,”
Phys. Rev. Lett., 69 3064 https://doi.org/10.1103/PhysRevLett.69.3064 PRLTAO 0031-9007
(1992).
Google Scholar
I. Pickering et al.,
“Diffraction anomalous fine structure: a new technique for probing local atomic environment,”
J. Am. Chem. Soc., 115 6302 https://doi.org/10.1021/ja00067a052 JACSAT 0002-7863
(1993).
Google Scholar
B. L. Henke, E. M. Gullikson and J. C. Davis,
“X-ray interactions: photoabsorption, scattering, transmission, and reflection at E=50−30000 eV, Z=1–92,”
At. Data Nucl. Data. Table, 54
(2), 181
–342 https://doi.org/10.1006/adnd.1993.1013
(1993).
Google Scholar
N. Kikuchi et al.,
“Atomic scattering factor of the ASTRO-H (Hitomi) SXT reflector around the gold’s L edges,”
Opt. Exp., 24 25548 https://doi.org/10.1364/OE.24.025548 OPEXFF 1094-4087
(2016).
Google Scholar
D. E. Graessle,
“Iridium optical constants for the Chandra X-ray Observatory from reflectance measurements of 0.05–12 keV,”
Proc. SPIE, 5165 469 https://doi.org/10.1117/12.506132 PSISDG 0277-786X
(2004).
Google Scholar
H. Awaki,
“Measuring the atomic scattering factors near the iridium L-edges for the Athena silicon pore optics reflector,”
J. Astron. Telesc. Instrum. Syst., 7 014001 https://doi.org/10.1117/1.JATIS.7.1.014001
(2021).
Google Scholar
R. L. Kelley et al.,
“The astro-H high resolution soft x-ray spectrometer,”
Proc. SPIE, 9905 99050V https://doi.org/10.1117/12.2232509
(2016).
Google Scholar
D. Barret et al.,
“The ATHENA X-ray integral field unit (X-IFU),”
Proc. SPIE, 10699 106991G https://doi.org/10.1117/12.2312409
(2018).
Google Scholar
M. J. Collon,
“Silicon pore optics development for ATHENA,”
Proc. SPIE, 9603 96030K https://doi.org/10.1117/12.2188988
(2015).
Google Scholar
S. Massahi et al.,
“Installation and commissioning of the silicon pore optics coating facility for the ATHENA mission,”
Proc. SPIE, 11119 111190F https://doi.org/10.1117/12.2528351
(2019).
Google Scholar
S. Goto et al.,
“Construction and commissioning of a 215-m-long beamline at SPring-8,”
Nucl. Instrum. Methods A, 467 682
–685 https://doi.org/10.1016/S0168-9002(01)00445-4
(2001).
Google Scholar
M. Yabashi,
“SPring-8 standard x-ray monochromators,”
Proc. SPIE, 3773 2
–13 https://doi.org/10.1117/12.370098
(1999).
Google Scholar
L. Nevot and P. Croce,
“Caractérisation des surfaces par réflexion rasante de rayons X. Application à l’ètude du polissage de quelques verres silicates,”
Rev. Phys. Appl., 15
(3), 761
–779 https://doi.org/10.1051/rphysap:01980001503076100ff RPHAAN 0035-1687
(1980).
Google Scholar
S. Massahi et al.,
“Investigation of boron carbide and iridium thin films, an enabling technology for future x-ray telescopes,”
Appl. Opt., 59 10902
–10911 https://doi.org/10.1364/AO.409453 APOPAI 0003-6935
(2020).
Google Scholar
J. H. Sinfelt and G. D. Meitzner,
“X-ray absorption edge studies of the electronic structure of metal catalysts,”
Acc. Chem. Res., 26
(1), 1
–6 https://doi.org/10.1021/ar00025a001 ACHRE4 0001-4842
(1993).
Google Scholar
J. A. Horsley,
“Relationship between the area of L2,3 x-ray absorption edge resonances and the d orbital occupancy in compounds of platinum and iridium,”
J. Chem. Phys., 76 1451 https://doi.org/10.1063/1.443105 JCPSA6 0021-9606
(1982).
Google Scholar
V. Monteseguro et al.,
“Phase stability and electronic structure of iridium metal at the megabar range,”
Sci. Rep., 9 8940 https://doi.org/10.1038/s41598-019-45401-x SRCEC3 2045-2322
(2019).
Google Scholar
T. K. Sham,
“L-edge x-ray-absorption systematics of the noble metals Rh, Pd, and Ag and the main-group metals In and Sn: a study of the unoccupied density of states in 4D elements,”
Phys. Rev. B., 31 1888
–1902 https://doi.org/10.1103/PhysRevB.31.1888
(1985).
Google Scholar
M. Honda et al.,
“A fluorescence XAFS measurement instrument in the soft x-ray region toward observation under operando conditions,”
Rev. Sci. Instrum., 86 035103 https://doi.org/10.1063/1.4913653
(2015).
Google Scholar
L. Tröger et al.,
“Full correction of the self-absorption in soft-fluorescence extended x-ray-absorption fine structure,”
Phys. Rev. B, 46 3283 https://doi.org/10.1103/PhysRevB.46.3283
(1992).
Google Scholar
B. Ravel and M. Newville,
“ATHENA, ARTEMIS, HEPHAESTUS: data analysis for X-ray absorption spectroscopy using IFEFFIT,”
J. Synchrotron Radiation, 12 537
–541 https://doi.org/10.1107/S0909049505012719
(2005).
Google Scholar
|